Tensile test of Dumet paper base paper for calcium chloride desiccant:
Test conditions: gauge length 150mm, sample width 15mm
Number of samples |
Maximum force£¨N£© |
Average force£¨N£© |
Elongation at break£¨%) |
1 |
62.92 |
45.91 |
38.229 |
2 |
62.17 |
45.53 |
39.618 |
3 |
52.76 |
39.59 |
30.482 |
4 |
54.85 |
40.60 |
29.561 |
5 |
57.16 |
42.50 |
29.709 |
6 |
63.47 |
46.91 |
34.225 |
7 |
53.79 |
40.18 |
30.173 |
8 |
56.64 |
42.65 |
30.79 |
9 |
59.67 |
43.90 |
34.744 |
10 |
62.44 |
45.89 |
35.314 |
Serial number |
Number of samples |
Heat sealing strength£¨N) |
¢Ù |
1 |
13.25 |
2 |
12.80 |
|
3 |
18.61 |
|
¢Ú |
1 |
17.89 |
2 |
17.47 |
|
3 |
12.56 |
|
¢Û |
1 |
15.12 |
2 |
13.61 |
|
3 |
17.01 |
|
¢Ü |
1 |
16.60 |
2 |
13.68 |
|
3 |
14.30 |
|
¢Ý |
1 |
17.79 |
2 |
15.02 |
|
3 |
16.37 |
Longitudinal sealing and heat sealing strength test of Dumet paper for calcium
chloride desiccant: Condition: sample width 15mm
Serial number |
Number of samples |
Heat sealing strength£¨N) |
¢Ù |
1 |
7.16 |
2 |
9.23 |
|
3 |
5.84 |
|
¢Ú |
1 |
10.80 |
2 |
8.00 |
|
3 |
8.06 |
|
¢Û |
1 |
8.22 |
2 |
13.91 |
|
3 |
13.50 |
|
¢Ü |
1 |
12.36 |
2 |
15.04 |
|
3 |
14.16 |
|
¢Ý |
1 |
14.04 |
2 |
15.09 |
|
3 |
10.34 |